Effect of Laser Surface Texturing Using a Surface Transition Machine on Bonding Strength to Zirconia Ceramic

Article information

J Korean Acad Pediatr Dent. 2025;52(3):302-311
Publication date (electronic) : 2025 August 22
doi : https://doi.org/10.5933/JKAPD.2025.52.3.302
Department of Pediatric Dentistry, College of Dentistry, Dankook University, Cheonan, Republic of Korea
Corresponding author: Jongsoo Kim Department of Pediatric Dentistry, College of Dentistry, Dankook University, 119, Dandae-ro, Dongnam-gu, Cheonan, 31116, Republic of Korea Tel: +82-41-550-0223 / Fax: +82-41-550-0118 / E-mail: jskim@dku.edu
Funding informationThis research was supported by Ceramic Technology Co., Ltd.
Received 2025 May 30; Revised 2025 July 9; Accepted 2025 July 11.

Abstract

The purpose of this study was to evaluate the effect of zirconia surface treatment using laser surface texturing performed with a Surface Transition Machine (STM). Zirconia specimens were fabricated in two shapes: 40 cylindrical specimens and square specimens. These were divided into two groups: the sandblasting group and the STM treatment group. Each group was bonded with either resin cement (Duo-Link) or resin-modified glass ionomer (RMGI) cement (RelyX Luting 2) after Z-Prime Plus primer application. The shear bond strength was measured using a universal testing machine, and the surface characteristics were analyzed using scanning electron microscopy and high-performance 3D digital microscopy. The group bonded with resin cement after STM treatment (48.4 ± 10.4 MPa) exhibited the highest shear bond strength, whereas the group bonded with RMGI cement after sandblasting (8.1 ± 1.5 MPa) exhibited the lowest. The STM treatment group showed significantly higher shear bond strength than the sandblasted group, and the Duo-Link group demonstrated significantly higher bond strength than the RelyX Luting 2 group. Surface observations showed that the STM treatment group exhibited rough surfaces and regularly patterned retentive structures. The surface roughness (Sa) was also significantly higher in the STM treatment group (13.3 ± 1.5 μm) than in the sandblasting group (7.08 ± 0.4 μm). In conclusion, STM treatment effectively improved the shear bond strength between zirconia and cement, particularly providing the highest bond strength when used with resin cement.

Introduction

Zirconia crowns are increasingly being selected as restorative materials because of the increase in aesthetic demands in pediatric treatment and their superior aesthetic properties, which provide high parental and child satisfaction compared to traditional metallic restorations [1,2]. Zirconia has excellent mechanical strength, wear resistance, and biocompatibility [3-6]. However, the surface of zirconia exhibits low adhesion owing to its chemical and physical characteristics. Zirconia has a chemically stable surface with a low surface energy [7-9] and low surface roughness, and it reduces mechanical retention with luting cement [10]. Effective adhesion requires appropriate surface treatments and adhesive systems [11]. Multiple surface treatment approaches have been developed to enhance zirconia bonding. Sandblasting with aluminum oxide (Al2O3) has been commonly used as a surface treatment method for increasing surface roughness [12,13]. However, studies have shown that sandblasting alone provides insufficient mechanical bonding strength and can induce microcracks and phase transformations, potentially degrading the mechanical properties of zirconia and leading to decreased longterm bonding strength [14-18].

To address the limitations of sandblasting, alternative surface modification approaches such as laser surface texturing have gained attention. Various laser systems have demonstrated the ability to create controlled surface patterns to improve the bonding characteristics [19].

A Surface Transition Machine (STM; Ceramic Technology co. Ltd., Seoul, Korea) is an advanced fiber laser technology used for the controlled surface modification of zirconia substrates. STM applies intense heat to the zirconia surface, generating explosive-like energy that modifies the surface morphology. This laser-induced surface modification process creates both micro- and macro-retention forms, thereby maximizing adhesion strength between zirconia and luting cements [20].

The purpose of this study was to investigate the effects of laser surface texturing using STM on the shear bond strength, analyze the surface morphology, and measure the surface roughness.

Materials and Methods

1. Materials

Resin and resin-modified glass ionomer (RMGI) cements were used in this study. Duo-Link (Bisco Inc., Schaumburg, IL, USA) was used as the resin cement and RelyX Luting 2 (3M ESPE, St. Paul, MN, USA) was used as the RMGI cement. Sandblasting was performed using 50 μm Al2O3. STM was used to determine the surface transition mechanisms. Z-Prime Plus (Bisco Inc., Schaumburg, IL, USA) was used as the primer. The materials used in this study are listed in the table below (Table 1).

Materials used in this study

2. Methods

1) Shear Bond Strength Test

Forty cylindrical zirconia ceramic specimens (6.0 mm in diameter, 5.0 mm in height) and 40 square zirconia ceramic specimens (10.0 mm × 10.0 mm × 5.0 mm) were prepared. Twenty cylindrical and 20 square specimens were surface-treated using STM that employs fiber laser technology to create retentive surface patterns, one hour before sintering. The remaining 20 cylindrical and 20 square specimens were treated with sandblasting using 50 μm Al2O3 particles at 3 bar pressure for 20 sec from a distance of 1 cm perpendicular to the surface.

Each surface treatment group (STM or sandblasting) was subdivided into two subgroups (n = 10 each) based on the type of cement used for bonding: Duo-Link or RelyX™ Luting 2 (Table 2).

Experimental group classification

Bonding was performed by applying cement to the flat bonding surface of each cylindrical zirconia specimen using different application methods depending on the cement type. For Duo-Link, the cement was applied using an automix syringe, whereas for RelyX™ Luting 2, equal amounts of pastes A and B were dispensed from the Clicker dispenser onto a mixing pad and mixed with a spatula for 20 sec in a 1 : 1 ratio before application. The cylindrical specimen was then placed vertically at the exact center of the corresponding square zirconia specimen. The alignment was standardized using a digital caliper and visual markers. Gentle finger pressure was applied initially, followed by the placement of a 500 g weight to maintain constant pressure during curing. Light curing was performed using a VALO™ X LED curing light (Ultradent Products Inc., South Jordan, UT, USA) in standard power mode with an intensity of 1000 mW/cm² and a wavelength range of 395 ‒ 480 nm. For the Duo-Link, light curing was performed for 3 sec, after which the excess cement extending beyond the cylindrical margin was removed using an explorer. Additional light curing was performed for 20 sec. For RelyX™ Luting 2, the mixed cement was light-cured for 5 sec; then, the excess cement was removed, followed by an additional 20 sec of light curing and 8 min of self-curing. All specimens were stored in distilled water at 37°C for 24 h before testing.

The shear bond strengths between the zirconia ceramic and the two types of cement were measured using a universal testing machine (QRUTS-S110, Quro, Yangju, Korea). The shear force was set at a crosshead speed of 1.0 mm/min and the maximum load until separation of the bonded cylindrical and square zirconia ceramic specimens was measured. This was converted to bonding strength per unit area (MPa).

2) Scanning Electron Microscopy Observation

To examine the microstructure of the zirconia ceramic specimens after surface treatment, cylindrical zirconia specimens identical to those used in the shear bond strength were prepared for each surface treatment group (STM treatment and sandblasting). Three specimens from each group were sputter-coated with platinum and observed using a scanning electron microscope (S-3000H, Hitachi, Marunouchi, Japan). The surface morphology was analyzed at magnifications of ×250, ×500, and × 2000. Representative images of the most characteristic surface features are shown.

3) Surface Observation and Surface Roughness Measurement Using High-Performance 3D Digital Microscopy

To examine the microstructure of the zirconia ceramic specimens after surface treatment, 10 additional cylindrical specimens were prepared for each surface treatment group (STM treatment and sandblasting). Surface morphology was evaluated using a high-performance 3D digital microscope (VHX-7000, Keyence, Osaka, Japan), and surface roughness (Sa) was quantitatively measured using profile measurement software (VHX-H5M, Keyence). To ensure reliable and reproducible data, surface roughness measurements were performed at three different locations on each specimen, and the median value was calculated and used as the representative value for each specimen.

3. Statistical Analysis

IBM SPSS 27.0 (SPSS Inc., Chicago, IL, USA) was used for statistical analysis. Shear bond strength was analyzed using the Kruskal-Wallis test with post-hoc Mann-Whitney U tests and Bonferroni correction. Surface roughness was compared using the Mann-Whitney U test.

Results

1. Shear Bond Strength

Shear bond strengths according to cement type and surface treatment method are presented (Table 3, Fig. 3). The STMDL group showed the highest shear bond strength at 48.4 ± 10.4 MPa, whereas the SbRXL group showed the lowest value at 8.1 ± 1.5 MPa. The STMDL and STMRXL groups exhibited significantly higher shear bond strengths than the SbDL and SbRXL groups. The SbDL and STMDL exhibited significantly higher shear bond strengths than those of the SbRXL and STMRXL groups.

Results of the shear bond strength test

Fig 3.

SEM images of surface-treated zirconia ceramic (magnification ×500). (A) Sandblasting, (B) STM treatment. STM: Surface Transition Machine.

2. Scanning Electron Microscopy Observation

The surfaces of the zirconia specimens after surface treatment were observed using scanning electron microscopy at 250×, 500×, and 2000× magnifications (Figs. 2, 3, and 4). The sandblasted zirconia surface exhibited crater-like microscopic irregularities of varying sizes formed by particle collisions. However, these structures were randomly distributed, lacked uniform patterns, and were not clearly defined. In contrast, the STMtreated surface exhibited a regularly arranged retentive structure with parallel linear grooves showing consistent spacing and unidirectional orientation. The STM-treated surfaces exhibited deeper and rougher topographical features than the sandblasted surfaces.

Fig 1.

Shear bond strength test.

Different superscript letters indicate statistically significant differences between groups (p < 0.0083).

Vertical bars represent the standard deviation.

SB: Sandblasting; STM: Surface Transition Machine; DL: Duo-Link cement; RXL: RelyX Luting2 cement.

Fig 2.

SEM images of surface-treated zirconia ceramic (magnification ×250). (A) Sandblasting, (B) STM treatment. STM: Surface Transition Machine.

Fig 4.

SEM images of surface-treated zirconia ceramic (magnification ×2000). (A) Sandblasting, (B) STM treatment. STM: Surface Transition Machine.

3. Surface observation and surface roughness measurement using high-performance 3D digital microscopy

The results of the observation of the surfaces of the zirconia specimens using a high-performance 3D digital microscope are shown (Figs. 5 and 6). The sandblasted zirconia specimens showed relatively uniform surface morphology with randomly distributed surface irregularities lacking directional orientation, whereas the STMtreated specimens exhibited increased surface roughness and organized linear microstructures with parallel groove formations. The side view of the STM-treated specimen shows V-shaped groove profiles with defined sidewalls and a consistent groove shape. The results of the surface roughness measurement experiments are presented (Table 5, Fig. 7). The Sa value of the STM treatment group was 13.3 ± 1.5 μm which was significantly higher than that of the sandblasted zirconia at 7.08 ± 0.4 μm (p= 0.0002).

Fig 5.

Optical microscopy images of surface-treated zirconia ceramic (magnification ×400). (A) Sandblasting, (B) STM treatment.

STM: Surface Transition Machine.

Fig 6.

Microscopic image showing a cross-sectional view of the STM-treated zirconia surface (×300).

STM: Surface Transition Machine.

Post hoc pairwise comparisons of shear bond strength using Mann-Whitney U tests with Bonferroni correction (adjusted α = 0.0083)

Surface roughness

Fig 7.

Results of the surface roughness (Sa) test.

Different superscript letters indicate statistically significant differences between groups (p < 0.05).

Vertical bars represent the standard deviation.

Sb: Sandblasting; STM: Surface Transition Machine.

Discussion

Numerous studies have been conducted to improve the bond strength between zirconia and luting cement. A high bond strength between the zirconia and cement was achieved when both chemical and mechanical treatment methods were applied. In this experiment, sandblasting and STM were used as the mechanical treatment methods, and Z-Prime Plus was applied to all groups as a chemical treatment.

The shear bond strength test is one of the methods used to evaluate the bonding ability of adhesive materials [21]. In this study, the STM treatment group showed a significantly higher shear bond strength than the sandblasted group for both the resin cement and RMGI cement. According to Yoon [20], in a shear bond strength experiment using resin cement, specimens treated with STM exhibited higher values than those treated with sandblasting. Several studies have reported that stronger mechanical bonding can be achieved on surfaces with micro-irregularities through surface treatment than on untreated zirconia [22,23]. SEM and high-performance 3D digital microscopy revealed that the STM treatment produced more distinct, regular, and repetitive surface patterns than sandblasting. These structures likely enhance the macro- and micro-retention by facilitating the formation of resin tags [24,25]. The STM-treated surface exhibited a significantly higher surface roughness than the sandblasted surface. A higher surface roughness results in smaller contact angles and higher wettability. This may also have contributed to the high shear bond strengths of the STMDL and STMRXL groups [26,27].

The STMDL and SbDL groups exhibited higher shear bond strengths than the STMRXL and SbRXL groups, regardless of the surface treatment method. Many studies have shown that resin cement exhibits a better bonding performance than RMGI cement for zirconia adhesion [28-34]. Resin cement provides high fracture resistance, increased retention, excellent aesthetics, marginal adaptation, and low microleakage [35-37]. Although studies have shown that RMGI provides a higher bond strength than glass ionomers [38], Piwowarczyk et al. [31] argued that, excluding resin cement, sufficient bonding strength cannot be achieved with RMGI, glass ionomer, or zinc phosphate cements. According to Lüthy et al. [39], zirconia restorations must have a bond strength of at least 10 ‒ 13 MPa for clinical viability. In this study, all experimental groups, except the SbRXL group, showed average shear bond strengths greater than 13 MPa, indicating clinical applicability. However, to withstand high masticatory forces and repeated stresses in the posterior teeth, a shear bond strength of over 30 MPa is required [40,41]. Therefore, for the effective adhesion of zirconia restorations, the use of resin cement along with STM treatment is considered appropriate.

In this experiment, Z-Prime Plus was applied to the zirconia specimens. Z-Prime Plus contains a 10-methacryloyloxydecyl dihydrogen phosphate (10-MDP) monomer. The 10-MDP primer treatment is effective for zirconia adhesion [38]. The bifunctional termini of MDP consist of long organic and hydrophobic chains [40]. The phosphate ester group of 10-MDP directly bonds with the hydroxyl groups of zirconia to form zirconium phosphate, resulting in a high bond strength [38,42,43]. The resin cement containing 10-MDP alone was not sufficient to ensure adhesion to zirconia without pretreatment. Treating the surface with a primer containing 10-MDP was effective in further improving the adhesion strength [44]. According to Yoon [20], a significantly improved shear bond strength was observed in the group where 10-MDP-containing primers were applied after sandblasting compared to the group with sandblasting alone. The groups treated with STM alone and STM followed by primer application showed significantly higher shear bond strengths than other groups. When comparing the STM treatment groups, the group treated with additional primers showed slightly higher bond strength values; however, this difference was not statistically significant.

STM offers various advantages for the surface treatment of zirconia. Unlike sandblasting, STM treatment does not require additional consumables such as Al2O3 and reduces the possibility of damage to zirconia [20]. Although sandblasting can induce microcracks and phase transformations [14,15], no notable microcracks were detected within the area observed using SEM. STM treatment may enhance the bonding strength of zirconia, reduce the risk of debonding, and improve the longterm clinical success rates. STM treatment can expand the range of treatment options that were previously limited by bond strength limitations, such as Maryland bridges, zirconia crowns, inlays, and onlays. It may also be useful in pediatric and adolescent patients with congenital tooth defects, tooth malformations, or enamel hypoplasia [45-47].

This study had some limitations. This study was conducted in a laboratory setting and did not fully replicate the conditions of the oral environment. Because longterm adhesion stability was not evaluated, additional research on the changes in bond strength over time is necessary. To assess long-term adhesion stability, thermocycling should be performed as it simulates the thermal stresses that occur in the oral environment over time. Furthermore, owing to the limited number of samples and types of cement, primers, and surface treat-ment methods used, further research on the optimal adhesion methods for zirconia is required.

Conclusion

In conclusion, this study evaluated the effects of zirconia surface treatment on the shear bond strength between RMGI and resin cement. The results showed that the STM treatment groups exhibited significantly higher shear bond strengths and surface roughness than the sandblasting treatment groups (p < 0.05). The highest bond strength was observed when bonded with the resin cement after STM treatment. STM treatment improves the bond strength of zirconia within the limitations of this in vitro study and may have potential for the clinical application of zirconia-based restorations in pediatric dentistry.

Notes

Acknowledgments

This research was supported by Ceramic Technology Co., Ltd.

Conflicts of Interest

The authors declare that zirconia specimens used in this study were provided by Ceramic Technology Co., Ltd. The company had no influence on the study design, data collection, analysis, or interpretation of the results. No financial support was received.

CRediT Authorship Contribution Statement

YongWoo Choi: Conceptualization, Investigation, Methodology, Formal analysis, Writing – original draft, Visualization. Jongbin Kim: Investigation, Data curation, Writing – review & editing, Validation. Mi Ran Han: Investigation, Data curation, Writing – review & editing, Validation. Jisun Shin: Investigation, Data curation, Writing – review & editing, Validation. Joonhaeng Lee: Investigation, Data curation, Writing – review & editing, Validation. Jongsoo Kim: Conceptualization, Supervision, Project administration, Funding acquisition, Resources, Writing – review & editing.

References

1. Alzanbaqi SD, Alogaiel RM, Alasmari MA, Al Essa AM, Khogeer LN, Alanazi BS, Hawsah ES, Shaikh AM, Ibrahim MS. Zirconia crowns for primary teeth: a systematic review and meta-analyses. Int J Environ Res Public Health 19:2838. 2022;
2. Salami A, Walia T, Bashiri R. Comparison of parental satisfaction with three tooth-colored full-coronal restorations in primary maxillary incisors. J Clin Pediatr Dent 39:423–428. 2015;
3. Hannink RH, Kelly PM, Muddle BC. Transformation toughening in zirconia-containing ceramics. J Am Ceram Soc 83:461–487. 2000;
4. Wei C, Gremillard L. Towards the prediction of hydrothermal ageing of 3Y-TZP bioceramics from processing parameters. Acta Materialia 144:245–256. 2018;
5. Evans AG. Perspective on the development of high-toughness ceramics. J Am Ceram Soc 73:187–206. 1990;
6. Walia T, Salami AA, Bashiri R, Hamoodi OM, Rashid F. A randomised controlled trial of three aesthetic full-coronal restorations in primary maxillary teeth. Eur J Paediatr Dent 15:113–118. 2014;
7. Wegner SM, Kern M. Long-term resin bond strength to zirconia ceramic. J Adhes Dent 2:139–147. 2000;
8. Qeblawi DM, Muñoz CA, Brewer JD, Monaco Jr EA. The effect of zirconia surface treatment on flexural strength and shear bond strength to a resin cement. J Prosthet Dent 103:210–220. 2010;
9. Yang L, Xie H, Meng H, Wu X, Chen Y, Zhang H, Chen C. Effects of Luting Cements and Surface Conditioning on Composite Bonding Performance to Zirconia. J Adhes Dent 20:549–558. 2018;
10. Borges GA, Sophr AM, De Goes MF, Sobrinho LC, Chan DC. Effect of etching and airborne particle abrasion on the microstructure of different dental ce-ramics. J Prosthet Dent 89:479–488. 2003;
11. Oliveira-Ogliari A, Collares FM, Feitosa VP, Sauro S, Ogliari FA, Moraes RR. Methacrylate bonding to zirconia by in situ silica nanoparticle surface deposition. Dent Mater 31:68–76. 2015;
12. Kim SH. Shear bond strength between zirconia and porcelain. J Technol Dent 33:1–6. 2011;
13. Su N, Yue L, Liao Y, Liu W, Zhang H, Li X, Wang H, Shen J. The effect of various sandblasting conditions on surface changes of dental zirconia and shear bond strength between zirconia core and indirect composite resin. J Adv Prosthodont 7:214–223. 2015;
14. Kern M, Wegner SM. Bonding to zirconia ceramic: adhesion methods and their durability. Dent Mater 14:64–71. 1998;
15. Chintapalli RK, Rodriguez AM, Marro FG, Anglada M. Effect of sandblasting and residual stress on strength of zirconia for restorative dentistry applications. J Mech Behav Biomed Mater 29:126–137. 2014;
16. Zhang Y, Lawn BR, Rekow ED, Thompson VP. Effect of sandblasting on the long-term performance of dental ceramics. J Biomed Mater Res B Appl Biomater 71:381–386. 2004;
17. Kim HK, Yoo KW, Kim SJ, Jung CH. Phase transformations and subsurface changes in three dental zirconia grades after sandblasting with various Al2O3 particle sizes. Materials 14:5321. 2021;
18. Lughi V, Sergo V. Low temperature degradation-aging-of zirconia: A critical review of the relevant aspects in dentistry. Dent Mater 26:807–820. 2010;
19. Han J, Zhang F, Van Meerbeek B, Vleugels J, Braem A, Castagne S. Laser surface texturing of zirconia-based ceramics for dental applications: A review. Mater Sci Eng C Mater Biol Appl 123:112034. 2021;
20. Yoon JY. Improving Zirconia-Resin Cement Bonding Through Laser Surface Texturing: A Comparative Study. Prosthesis 7:19. 2025;
21. Ismail AM, Bourauel C, ElBanna A, Salah Eldin T. Micro versus macro shear bond strength testing of dentin-composite interface using chisel and wireloop loading techniques. Dent J 9:140. 2021;
22. Aboushelib MN, Matinlinna JP, Salameh Z, Ounsi H. Innovations in bonding to zirconia-based materials: Part I. Dent Mater 24:1268–1272. 2008;
23. Shin CH, Hwang SS, Han KS. Shear bond strength of veneering ceramic and zirconia core according to the surface treatments. J Dent Hyg Sci 13:487–492. 2013;
24. Carek A, Slokar Benić L, Komar D, Krebelj E. Roughness of the Surface of Zirconia Reinforced Lithium Disilicate Ceramic treated by different procedures. Materials 16:265. 2022;
25. Grigore A, Spallek S, Petschelt A, Butz B, Spiecker E, Lohbauer U. Microstructure of veneered zirconia after surface treatments: a TEM study. Dent Mater 29:1098–1107. 2013;
26. Yekta-Fard M, Ponter AB. Factors affecting the wettability of polymer surfaces. J Adhes Sci Technol 6:253–277. 1992;
27. Sismanoglu S, Yildirim-Bilmez Z, Erten-Taysi A, Ercal P. Influence of different surface treatments and universal adhesives on the repair of CAD-CAM composite resins: An in vitro study. J Prosthet Dent 124:238.e1–9. 2020;
28. Lee J, Park H, Lee J, Seo H. Shear bonding strength of three cements luted on pediatric zirconia crowns and dentin of primary teeth. J Korean Acad Pediatr Dent 45:314–323. 2018;
29. Cho SH, Cho IH, Lee JH, Nam KY, Hwang SH, Kim JB. In vitro evaluation of shear bond strengths of zirconia ceramic with various types of cement after thermocycling on bovine dentin surface. J Oral Rehabil Appl Sci 23:249–257. 2007;
30. Khalil RJ, Al-Shamma AM. Micro-shear bond strength of a novel resin-modified glass ionomer luting cement (eRMGIC) functionalized with organophosphorus monomer to different dental substrates. Heliyon 10:e30851. 2024;
31. Piwowarczyk A, Lauer HC, Sorensen JA. The shear bond strength between luting cements and zirconia ceramics after two pre-treatments. Oper Dent 30:382–388. 2005;
32. Szalay ER, Gómez AG, Ibarra JG, Romero IM, Muro KM. Comparative study of displacement resistance of four zirconia cements. Rev Odont Mex 21:e227–e232. 2017;
33. Bindl A, Lüthy H, Mörmann WH. Thin-wall ceramic CAD/CAM crown copings: strength and fracture pattern. J Oral Rehabil 33:520–528. 2006;
34. Zhang W, Masumi SI, Song XM. Bonding property of two resin-reinforced glass-ionomer cements to zirconia ceramic. Quintessence Int 41:e132–e140. 2010;
35. Blatz MB, Sadan A, Kern M. Resin-ceramic bonding: a review of the literature. J Prosthet Dent 89:268–274. 2003;
36. Blatz MB, Chiche G, Holst S, Sadan A. Influence of surface treatment and simulated aging on bond strengths of luting agents to zirconia. Quintessence Int 38:745–753. 2007;
37. Palacios RP, Johnson GH, Phillips KM, Raigrodski AJ. Retention of zirconium oxide ceramic crowns with three types of cement. J Prosthet Dent 96:104–114. 2006;
38. De Angelis F, D'Arcangelo C, Buonvivere M, Rondoni GD, Vadini M. Shear bond strength of glass ionomer and resin-based cements to different types of zirconia. J Esthet Restor Dent 32:806–814. 2020;
39. Lüthy H, Loeffel O, Hammerle CH. Effect of thermocycling on bond strength of luting cements to zirconia ceramic. Dent Mater 22:195–200. 2006;
40. Yue X, Hou X, Gao J, Bao P, Shen J. Effects of MDPbased primers on shear bond strength between resin cement and zirconia. Exp Ther Med 17:3564–3572. 2019;
41. Lim MJ, Yu MK, Lee KW. The effect of continuous application of MDP-containing primer and luting resin cement on bond strength to tribochemical silica-coated Y-TZP. Restor Dent Endod 43:e19. 2018;
42. Aboushelib MN, Feilzer AJ, Kleverlaan CJ, Salameh Z. Partial-retainer design considerations for zirconia restorations. Quintessence Int 41:41–18. 2010;
43. Khan AA, Al Kheraif A, Jamaluddin S, Elsharawy M, Divakar DD. Recent trends in surface treatment methods for bonding composite cement to zirconia: a review. J Adhes Dent 19:7–19. 2017;
44. Ahn JS, Yi YA, Lee Y, Seo DG. Shear Bond Strength of MDP-Containing Self-Adhesive Resin Cement and Y-TZP Ceramics: Effect of Phosphate Monomer-Containing Primers. Biomed Res Int 2015:389234. 2015;
45. Alhissan AS, Pani SC. Factors influencing the survival of preformed zirconia crowns in children treated under general anesthesia. Int J Dent 2021:5515383. 2021;
46. Quigley NP, Loo DS, Choy C, Ha WN. Clinical efficacy of methods for bonding to zirconia: A systematic review. J Prosthet Dent 125:231–240. 2021;
47. Yangdol P, Kalra N, Tyagi R, Khatri A, Khandelwal D, Kulkarni S, Kulood K. Modified zirconia-bonded M-bridge for prosthetic rehabilitation of missing anterior tooth in a young adolescent. Int J Oral Health Sci 13:51–54. 2023;

Article information Continued

Fig 1.

Shear bond strength test.

Different superscript letters indicate statistically significant differences between groups (p < 0.0083).

Vertical bars represent the standard deviation.

SB: Sandblasting; STM: Surface Transition Machine; DL: Duo-Link cement; RXL: RelyX Luting2 cement.

Fig 2.

SEM images of surface-treated zirconia ceramic (magnification ×250). (A) Sandblasting, (B) STM treatment. STM: Surface Transition Machine.

Fig 3.

SEM images of surface-treated zirconia ceramic (magnification ×500). (A) Sandblasting, (B) STM treatment. STM: Surface Transition Machine.

Fig 4.

SEM images of surface-treated zirconia ceramic (magnification ×2000). (A) Sandblasting, (B) STM treatment. STM: Surface Transition Machine.

Fig 5.

Optical microscopy images of surface-treated zirconia ceramic (magnification ×400). (A) Sandblasting, (B) STM treatment.

STM: Surface Transition Machine.

Fig 6.

Microscopic image showing a cross-sectional view of the STM-treated zirconia surface (×300).

STM: Surface Transition Machine.

Fig 7.

Results of the surface roughness (Sa) test.

Different superscript letters indicate statistically significant differences between groups (p < 0.05).

Vertical bars represent the standard deviation.

Sb: Sandblasting; STM: Surface Transition Machine.

Table 1.

Materials used in this study

Product Composition Manufacturer
Duo-Link Bis-GMA, TEGDMA, UDMA glass filler (filler content: 61.9 ± 0.43 wt%) Bisco Inc., Schaumburg, IL, USA
RelyX Luting 2 Paste A: fluoroaluminosilicate (FAS) glass, proprietary reducing agent, HEMA, water, opacifying agent GC Corporation, Tokyo, Japan
Paste B: methacrylated polycarboxylic acid, BisGMA, HEMA, water, potassium persulfate, zirconia silica filler
Z-Prime Plus Biphenyl dimethacrylate, MDP, ethanol Bisco Inc., Schaumburg, IL, USA

Bis-GMA: bisphenol-A-glycidyl methacrylate; TEGDMA: triethylene glycol dimethacrylate; UDMA: urethane dimethacrylate; HEMA: 2-hydroxyethyl methacrylate; MDP: methacryloyloxydecyl dihydrogen phosphate.

Table 2.

Experimental group classification

Group Surface Treatment Cement
SbDL Sandblasting Duo-Link
SbRXL Sandblasting RelyX Luting 2
STMDL STM treatment Duo-Link
STMRXL STM treatment RelyX Luting 2

Sb: Sandblasting; STM: Surface transition machine; DL: Duo-Link cement; RXL: RelyX Luting2 cement.

Table 3.

Results of the shear bond strength test

Group N Mean ± Standard Deviation
SbDL 10 29.8 ±6.2a
SbRXL 10 8.1 ± 1.5b
STMDL 10 48.4 ± 10.4c
STMRXL 10 13.4 ± 2.5d

Unit: MPa.

Sb: Sandblasting; STM: Surface transition machine; DL: Duo-Link cement; RXL: RelyX Luting 2 cement.

Kruskal-Wallis test: p < 0.001.

Different superscript letters indicate significant differences from post hoc Mann-Whitney U tests with Bonferroni correction (adjusted α = 0.0083).

Table 4.

Post hoc pairwise comparisons of shear bond strength using Mann-Whitney U tests with Bonferroni correction (adjusted α = 0.0083)

Comparison p value
SbDL vs SbRXL 0.0002
SbDL vs STMDL 0.0003
SbDL vs STMRXL 0.0002
SbRXL vs STMDL 0.0002
SbRXL vs STMRXL 0.0003
STMDL vs STMRXL 0.0002

SB: Sandblasting; STM: Surface Transition Machine; DL: Duo-Link cement; RXL: RelyX Luting2 cement.

Table 5.

Surface roughness

Group N Mean ± Standard Deviation p value
Sb 10 7.1 ± 0.4a 0.0002
STM 10 13.3 ± 1.5b

Unit: MPa.

Sb: Sandblasting, STM: Surface Transition Machine.

p value from the Mann-Whiteney test.