Evaluation of Shear Bond Strength of Submicron Polycrystalline Alumina Ceramic with Different Surface Treatments and Luting Cements

Article information

J Korean Acad Pediatr Dent. 2025;52(4):425-436
Publication date (electronic) : 2025 November 25
doi : https://doi.org/10.5933/JKAPD.2025.52.4.425
Department of Pediatric Dentistry, College of Dentistry, Dankook University, Cheonan, Republic of Korea
Corresponding author: Jongbin Kim Department of Pediatric Dentistry, College of Dentistry, Dankook University, 119 Dandae-ro, Dongnam-gu, Cheonan, 31116, Republic of Korea Tel: +82-41-550-3081 / Fax: +82-41-559-7839 / E-mail: Jbkim0222@dankook.ac.kr
Received 2025 June 30; Revised 2025 July 30; Accepted 2025 August 4.

Abstract

Submicron polycrystalline alumina ceramic offers excellent mechanical strength and translucency, making it a promising material for pediatric crown restorations. However, due to its acid resistance and low surface energy, reliable bonding requires appropriate surface treatments and selection of compatible cement materials. This study aimed to evaluate the shear bond strength of submicron polycrystalline alumina ceramics subjected to various surface treatments and bonded with different types of luting cements. Ninety specimens were divided into three surface treatment groups: no treatment, sandblasting, and Rocatec treatment. Each group was further subdivided by cement type: glass ionomer (GI) cement (GC Fuji I), resin-modified glass ionomer (RMGI) cement (RelyX Luting 2), and self-adhesive resin cement (RelyX U200). Shear bond strength was measured using a universal testing machine, and failure modes were analyzed using scanning electron microscopy. The combination of Rocatec treatment and self-adhesive resin cement exhibited the highest bond strength. Self-adhesive resin cement demonstrated significantly higher bond strength than the other cements under all surface conditions (p < 0.017). Within the self-adhesive resin and RMGI cement groups, shear bond strength varied significantly by surface treatment (p < 0.017), while no significant difference was found in GI cement group (p > 0.017). Adhesive failures occurred only in untreated groups, whereas cohesive and mixed failures appeared exclusively in surface-treated groups. Within the limitations of this in vitro study, Rocatec treatment with self-adhesive resin cement was the most effective bonding strategy for submicron polycrystalline alumina ceramics.

Introduction

In recent years, the increasing demand for esthetic restorations, along with advancements in dental laboratory technologies that have improved the physical properties and marginal fit of ceramic restorations, has led to a substantial rise in the use of all-ceramic restorations. In pediatric dentistry, parents are also showing a growing preference for prefabricated zirconia crowns. However, zirconia presents certain drawbacks, including high opacity and potential for increased wear on opposing dentition[1].

As a potential solution, submicron polycrystalline alumina ceramics have garnered increasing attention. This recently developed material offers the advantage of simultaneously achieving higher translucency and superior mechanical strength compared to zirconia and lithium disilicate glass ceramics[2,3]. Its high translucency not only enhances esthetic outcomes but also improves the efficiency of light polymerization of resin cements, contributing to clinical effectiveness. Furthermore, unlike zirconia, it exhibits resistance to low-temperature degradation and possesses a lower coefficient of thermal expansion, providing additional benefits in terms of long-term durability[4,5].

The clinical applications of submicron polycrystalline alumina ceramics are expanding to include high-strength single crowns and copings, orthodontic brackets, bridge frameworks, veneers, and inlay/onlay restorations. These developments indicate the material’s potential as a more esthetic and durable restorative option for pediatric patients[5,6].

However, polycrystalline alumina ceramics exhibit inherently low surface energy and chemical inertness, which limit their bonding strength with luting cements[7-9]. Therefore, achieving effective adhesion between submicron polycrystalline alumina ceramics and luting agents requires not only appropriate surface treatment but also careful selection of the cement.

Representative surface treatment methods include sandblasting and the Rocatec system (3M ESPE, St. Paul, MN, USA). Sandblasting involves the high-pressure application of alumina particles to increase surface roughness, thereby enhancing mechanical retention. The Rocatec system, on the other hand, involves blasting the surface with silica-coated alumina particles to form a silica layer, followed by the application of a silane coupling agent. This dual approach improves both mechanical interlocking and chemical bonding[8].

In addition, the choice of luting cement plays a critical role in bonding performance. Although traditional cements such as zinc phosphate and glass ionomer have been used for polycrystalline ceramics, their limited chemical affinity to the ceramic surface often results in suboptimal bond strength. In contrast, resin cements containing functional monomers such as Bis-GMA, 4-META, MDP, and methacrylated phosphoric ester monomers have been introduced in recent years. These monomers facilitate chemical bonding to the ceramic surface and have been reported to yield significantly higher bond strengths[10-13].

However, some studies on zirconia crowns have reported no significant difference in bond strength between resin-modified glass ionomer cements and resin cements containing functional monomers, suggesting that the optimal choice of cement may vary depending on the type of ceramic used[14,15]. Therefore, cement selection should be considered in conjunction with the surface treatment method of the ceramic. Fundamental studies based on these factors are essential for enhancing the clinical applicability of ceramic materials.

In line with this perspective, the present study included not only resin cements containing functional monomers but also conventional glass ionomer cement as a control group, given its continued widespread use in pediatric dentistry despite its relatively low bonding performance. In addition, a resin-modified glass ionomer cement, which demonstrates improved physical properties and bonding potential compared to traditional glass ionomer cement, was also evaluated. Accordingly, this study aimed to evaluate the shear bond strength of submicron polycrystalline alumina ceramics by applying various surface treatment methods in combination with three commonly used luting cements in clinical practice. By analyzing the bond strength of each combination, this study sought to assess the potential applicability of this material as a restorative option for pediatric crowns.

Materials and Methods

1. Materials

The materials used in this study are listed in Tables 1 and 2. Specimens were fabricated using 99.99% pure submicron polycrystalline alumina ceramics. Three types of luting cements were employed: glass ionomer (GI) (GC Fuji I, GC Corporation, Tokyo, Japan), resin-modified glass ionomer (RMGI) (RelyX Luting 2, 3M ESPE), and self-adhesive resin cement (RelyX U200, 3M ESPE). For surface treatments, 110 μm alumina particles (Rocatec Pre, 3M ESPE) and 110 μm silica-coated alumina particles (Rocatec Plus, 3M ESPE) were used.

Compositions and manufacturers of cement used in this study

Compositions and manufacturers of surface treatment materials in this study

2. Methods

1) Fabrication of submicron polycrystalline alumina ceramic specimens

The submicron polycrystalline alumina ceramic specimens used in this study were fabricated using high-purity fine powder with an average particle size of less than 0.15 μm (99.99% Al2O3, Grade TMDAR; Taimei Chemicals Co., Ltd., Japan). To prepare the feedstock suitable for Ceramic Injection Molding (CIM), the ceramic powder was homogeneously mixed with a paraffin-based wax and a polymer-based binder in a predetermined ratio.

To form the specimens, a disk-shaped mold with a diameter of 10.0 mm and a thickness of 2.0 mm was fabricated. The green bodies were produced by injecting the prepared feedstock into the mold under an average injection pressure of 1500 kgf/cm². The molded specimens then underwent thermal debinding, during which temperature was gradually increased to remove the paraffin and polymer-based binder components.

The debinded green bodies were sintered in a furnace by heating at a rate of 5°C/min up to 1500°C, followed by holding at the peak temperature for 5 hours to complete the sintering process. Subsequently, the specimens underwent a hot isostatic pressing (HIP) process to eliminate residual porosity and to enhance the density and mechanical properties of the material.

Ninety specimens fabricated through this process were embedded in self-curing acrylic resin within rectangular molds measuring 18.5 × 18.5 × 5.5 mm for shear bond strength testing (Fig. 1). The specimens were divided into three groups (n = 30 each) based on the surface treatment method, and further subdivided into three subgroups (n = 10 each) according to the type of cement used, resulting in nine experimental groups (Table 3).

Fig 1.

Disk-shaped submicron polycrystalline alumina ceramic specimen.

Experimental group classification

2) Surface treatment of submicron polycrystalline alumina ceramic specimens

For the sandblasting group, the specimen surfaces were treated by blasting 110 μm alumina particles perpendicularly for 10 seconds at a pressure of 4 bar from a distance of 10 mm. For the Rocatec group, the specimens first underwent sandblasting under the same conditions, followed by an additional perpendicular application of silica-coated 110 μm alumina particles at a pressure of 2.8 bar for 10 seconds from a distance of 10 mm. After all surface treatments, the specimens were ultrasonically cleaned for 5 minutes to remove residual particles and then dried prior to subsequent procedures. In the Rocatec group, a silane primer (Monobond N, Ivoclar Vivadent, Schaan, Liechtenstein) was additionally applied to the treated surfaces in accordance with the manufacturer’s instructions[16,17].

3) Cementation and storage of specimens

For cementation, a Teflon mold with a diameter of 5.0 mm and a height of 3.0 mm was used to apply the cement onto the surface of the submicron polycrystalline alumina ceramic specimens. For the glass ionomer cement (GC Fuji I, GC Corporation), the powder and liquid components were mixed at a 1 : 2 ratio for 20 seconds and allowed to self-cure for 7.5 minutes. The resin-modified glass ionomer cement (RelyX Luting 2, 3M ESPE) was prepared by mixing paste A and paste B at a 1 : 1 ratio for 20 seconds, followed by self-curing for 8 minutes. The self-adhesive resin cement (RelyX U200, 3M ESPE) was applied within the Teflon mold and light-cured using an LED curing unit (B&LiteS, B&L Biotech, Ansan, Korea) at an intensity of 1,000 mW/cm² from five directions perpendicularly for 20 seconds each, totaling 100 seconds. After cementation, all specimens were stored in a humidified incubator at 37°C for 48 hours (TH3-PE, JEIO TECH, Daejeon, Korea).

4) Shear bond strength measurement

The shear bond strength between the submicron polycrystalline alumina ceramic and the three types of luting cements was measured using a universal testing machine (QRUTS-S110, Quro, Yangju, Korea). A shear force was applied at a crosshead speed of 1.0 mm/min until debonding occurred, and the maximum load at failure was recorded. The value was then converted to bond strength in megapascals (MPa) based on the bonded surface area (Fig. 2).

Fig 2.

Schematic diagram of the shear bond strength test.

UTM: universal testing machine.

5) Scanning electron microscopy (SEM) evaluation

To evaluate the surface microstructure after surface treatment, one additional specimen from each surface treatment group was sputter-coated with platinum and observed at 1,000× magnification using a scanning electron microscope (S-3000H, Hitachi, Marunouchi, Japan). Following the shear bond strength test, the failure surfaces were examined at 200× magnification to classify the failure modes. The failure modes were categorized as adhesive failure, cohesive failure, or mixed failure.

3. Statistical analysis

A total of nine experimental groups were established to analyze differences in shear bond strength. These groups were formed by combining three surface treatment methods (no treatment, sandblasting, and Rocatec treatment) with three types of luting cements (GI, RMGI, and self-adhesive resin), with ten specimens included in each group (n = 10). The shear bond strength data satisfied the assumption of normality but did not meet the assumption of homogeneity of variance. Therefore, the Kruskal-Wallis test was used as a non-parametric method to assess group differences, with a significance level set at α = 0.05. When significant differences were found, pairwise comparisons were performed using the Mann- Whitney U test, and Bonferroni correction was applied to adjust for multiple comparisons, resulting in a corrected significance level of α = 0.017. For the analysis of failure modes, which were treated as categorical variables, Fisher’s exact test was used with a significance level of α = 0.05. All statistical analyses were conducted using IBM SPSS Statistics version 29.0 (IBM SPSS Inc., Chicago, IL, USA).

Results

1. Shear bond strength

The results of shear bond strength according to surface treatment methods and cement types are presented in Table 4 and illustrated in Fig. 3 and Fig. 4. Self-adhesive resin cement combined with Rocatec treatment showed the highest shear bond strength (10.24 MPa), followed by the same cement with sandblasting (6.30 MPa). Under each surface treatment condition, self-adhesive resin cement showed significantly higher bond strength than RMGI cement, which in turn was significantly higher than GI cement (p < 0.001; Table 4, Fig. 4). GI cement exhibited the lowest bond strength overall, ranging from 0.07 MPa (no treatment) to 0.15 MPa (Rocatec treatment), with no statistically significant differences among the surface treatment methods (p > 0.017; Table 4, Fig. 3). Meanwhile, both RMGI and self-adhesive resin cement showed significant differences among surface treatments, with the highest shear bond strength observed with Rocatec treatment, followed by sandblasting and then no treatment (p < 0.001; Table 4, Fig. 3).

Shear bond strength (MPa) of various cements according to surface treatment

Fig 3.

Effect of different surface treatments on the shear bond strength (MPa) of various luting cements. Groups sharing the same letter are not significantly different. Error bars represent standard deviation.

No: No treatment; Sb: Sandblasting; Ro: Rocatec treatment; GCF: GC Fuji I cement; RXL: RelyX Luting 2 cement; RXU: RelyX U200 cement.

Fig 4.

Effect of different luting cements on the shear bond strength (MPa) of surface-treated submicron polycrystalline alumina specimens. Groups sharing the same letter are not significantly different. Error bars represent standard deviation.

No: No treatment; Sb: Sandblasting; Ro: Rocatec treatment; GCF: GC Fuji I cement; RXL: RelyX Luting 2 cement; RXU: RelyX U200 cement.

2. Scanning electron microscopy (SEM)

The surfaces of the alumina ceramic specimens after surface treatment were examined using a scanning electron microscope (SEM) at 1,000× magnification (Fig. 5). In the no-treatment group, a relatively uniform and flat surface was observed, characterized by a consistent particle structure. In contrast, the sandblasting group showed a rough texture with irregular surface indentations caused by the alumina particle impact. The Rocatec treatment group exhibited an even rougher surface with a silica layer fused to the surface, confirming the characteristic effects of the Rocatec treatment.

Fig 5.

SEM images of surface-treated submicron polycrystalline alumina ceramic (magnification ×1,000). (A) No surface treatment, (B) Sandblasting, (C) Rocatec treatment.

Following shear bond strength testing, the fracture surfaces were analyzed using SEM. In the no-treatment group, all specimens exhibited adhesive failure, with flat and smooth surfaces observed (Fig. 6A). In contrast, one specimen each from the sandblasting and Rocatec treatment groups cemented with self-adhesive resin cement showed cohesive failure, indicating that fracture occurred within the resin cement (Fig. 6 and 7). Statistical analysis revealed that the Rocatec treatment group showed a significantly higher proportion of mixed failures compared to the no-treatment group (p= 0.010). In addition, both the self-adhesive resin cement and RMGI groups exhibited significantly higher proportions of mixed failures than the GI group (p= 0.024, respectively).

Fig 6.

SEM images after the shear bond strength test showing failure mode on submicron polycrystalline alumina ceramic (magnification ×200). (A) Adhesive failure on surfaces with no treatment, (B) Mixed failure on surfaces treated by sandblasting, (C) Cohesive failure treated by Rocatec treatment.

Fig 7.

Comparison of the failure modes of polycrystalline alumina ceramics according to different surface treatments and luting cements.

No: No surface treatment; Sb: Sandblasting; Ro: Rocatec treatment; GCF: GC Fuji I cement; RXL: RelyX Luting 2 cement; RXU: RelyX U200 cement.

Discussion

With recent advances in dental laboratory technology, high-purity polycrystalline alumina ceramics with an average particle size of less than 0.15 μm have been developed. Compared to conventional zirconia, these materials offer superior translucency, a lower coefficient of thermal expansion, and resistance to low-temperature degradation, making them suitable for fulfilling both esthetic and durability requirements. Currently, submicron polycrystalline alumina ceramics are being increasingly applied in various dental restorations, including single crowns, orthodontic brackets, frameworks, veneers, and inlays/onlays. However, to enable their application as restorative materials for pediatric crowns, further studies on surface treatment and cementation protocols are required[18,19].

Polycrystalline alumina ceramics exhibit low surface energy and chemical inertness, making conventional treatments such as silanization or hydrofluoric acid etching ineffective for bonding[20-22]. Therefore, appropriate surface treatments and cement selection that promote either mechanical or chemical adhesion are critical. Among various surface treatment methods, sandblasting enhances surface roughness and improves mechanical retention. Numerous studies have reported that sandblasting increases surface roughness and, consequently, bond strength[20,23,24]. Awliya et al.[20] reported that sandblasting with 50 μm alumina particles on polycrystalline alumina surfaces resulted in higher bond strength compared to hydrofluoric acid etching or polishing with diamond burs. Similarly, Blatz et al.[23] reported that resin cement bonded to alumina surfaces treated with 50 μm alumina particles maintained high bond strength even after 180 days of storage.

However, as noted by Phark et al.[25], if the ceramic already contains micro-porosities from the manufacturing process, sandblasting may reduce bond strength by eliminating these micro-retentive features. Thus, it is important to apply sandblasting appropriately according to the surface condition. In the present study, the submicron polycrystalline alumina ceramics used had a smoothly machined surface, and sandblasting improved bond strength in all cement groups except GI cement, compared to specimens with no surface treatment.

Rocatec treatment involves the airborne particle abrasion of silica-coated alumina particles to form a silica layer on the ceramic surface, followed by the application of a silane primer to promote chemical bonding. Even in ceramics that do not inherently contain silica, such as polycrystalline alumina or zirconia, this process enables the formation of a silica layer. The alkoxy groups (–Si–OR) of the silane react with the hydroxyl groups (–OH) on the silica surface to form stable Si–O–Si bonds. Additionally, the methacrylate end of the silane molecule can copolymerize with the methacrylate monomers present in the resin cement, establishing a chemical linkage between the ceramic and the cement.

Valandro et al.[26] reported that the Rocatec treatment was more effective than sandblasting, and a study by Lin et al.[27] also demonstrated that Rocatec treatment significantly improved the bonding strength of resin cements. In the present study, both self-adhesive resin and RMGI cement exhibited higher shear bond strength when combined with Rocatec treatment compared to sandblasting or no treatment. Notably, the combination of self-adhesive resin cement with Rocatec treatment yielded the highest bond strength. However, RMGI cement showed comparatively lower values, which can be attributed to differences in their chemical compositions. Self-adhesive resin cement contains methacrylate monomers with phosphoric acid groups, which are capable of forming strong chemical bonds with the hydroxyl groups (–OH) on the alumina surface through P–O–Al bonding or hydrogen bonding interactions[28,29]. In contrast, RelyX Luting (3M ESPE) 2 is a resin-modified glass ionomer cement containing HEMA, which may form hydrogen bonds with the ceramic surface. However, due to its high hydrophilicity and poor water resistance, it exhibits limited long-term interfacial stability[30,31]. In comparison, GC Fuji I (GC Corporation) is a conventional glass ionomer cement that does not contain methacrylate groups or functional monomers, resulting in minimal chemical interaction with the ceramic surface[32]. In addition, its high viscosity and prolonged setting time may compromise mechanical retention, which likely explains the lowest bond strength observed in this study.

Failure mode analysis also revealed cohesive failures in the sandblasting and Rocatec treatment groups cemented with self-adhesive resin cement, suggesting the combined effect of strong chemical bonding and mechanical retention[33]. In contrast, only adhesive failures were observed in all groups cemented with GI cement, indicating a lack of effective bonding to the ceramic surface[11,34].

This study has several limitations. First, this study did not evaluate the long-term changes in bonding strength of the cements. In the actual oral environment, bonding durability can deteriorate over time due to factors such as moisture absorption, temperature fluctuations, and mechanical stress. The water resistance and chemical stability of the cement play a critical role in maintaining long-term adhesion[35,36]. Blatz et al.[23] reported that bond strength may vary over time depending on the type of surface treatment and functional monomers used. In particular, cements without functional monomers exhibited a significant decrease in bond strength after long-term water storage and thermocycling, whereas cements containing functional monomers such as MDP or phosphoric acid ester maintained relatively stable adhesion. These findings suggest that long-term evaluations that consider both the chemical composition of the cement and its stability in moist environments are necessary in addition to short-term bond strength testing.

In addition, smoothly machined polycrystalline alumina ceramics were used during specimen fabrication to create a stable surface, which may have contributed to the overall lower bond strength. Although there is no established standard for the required bond strength of pediatric crowns, Lüthy et al.[12] suggested that a clinically acceptable threshold for shear bond strength ranges from 10 to 13 MPa, and ISO 10477 recommends a minimum of 5 MPa[37]. Based on the results of this study, the combinations of resin cement with either sandblasting or Rocatec treatment met the suggested bond strength criteria. Thus, for submicron polycrystalline alumina ceramics to be clinically applicable as pediatric crowns, surface activation of the internal crown surface should be considered during the fabrication process.

Lastly, this study focused on identifying overall bonding trends based on cement type (GI, RMGI, and self-adhesive resin) and surface treatment method, rather than comparing the performance of different resin cements. Although the results demonstrated that the combination of Rocatec treatment and self-adhesive resin cement achieved the highest bond strength, this outcome was somewhat predictable considering the chemical composition and adhesive characteristics of the materials. Previous studies have shown that bonding performance may vary depending on the type and concentration of functional monomers present in resin cements[13,30,31]. Therefore, direct comparison among various commercial resin cements with different monomer formulations could provide more detailed insights into selecting appropriate luting agents for clinical applications. Future studies should aim to investigate the effects of different functional monomers on long-term adhesion and their interaction with surface-treated alumina ceramics under simulated intraoral conditions.

Furthermore, to enhance clinical applicability, future studies should comprehensively evaluate various clinical factors such as occlusal wear, fracture resistance, amount of tooth reduction, marginal adaptation, and color stability.

Conclusion

This study evaluated the shear bond strength of submicron polycrystalline alumina ceramics according to different surface treatments and types of luting cements. The highest bond strength was observed in the group bonded with self-adhesive resin cement following Rocatec treatment, followed by the group treated with sandblasting and bonded with self-adhesive resin cement.

Among the three cements, self-adhesive resin cement consistently showed significantly higher bond strength across all surface treatment conditions, followed by RMGI and GI cement. Similarly, a comparison of surface treatment methods revealed that Rocatec treatment resulted in the highest bond strength, followed by sandblasting and then no treatment.

According to the failure mode analysis, all specimens in the untreated group exhibited adhesive failure, indicating weak interfacial bonding. In contrast, mixed failures and cohesive failures were observed in the sandblasting and Rocatec treatment groups bonded with self-adhesive resin cement, suggesting that surface treatments enhanced both mechanical retention and chemical bonding.

These findings indicate that the combination of surface treatment and cement type plays a critical role in achieving durable adhesion to submicron polycrystalline alumina ceramics and support their potential clinical application as a material for pediatric crowns.

Notes

Conflicts of Interest

The authors have no potential conflicts of interest to disclose.

CRediT authorship contribution statement

Yerim Song: Data curation, Formal analysis, Investigation, Methodology, Visualization, Writing - Original Draft, Writing - Review & Editing. Jongsoo Kim: Resources, Validation, Writing - Review & Editing. Joonhaeng Lee: Validation, Writing - Review & Editing. Miran Han: Validation, Writing - Review & Editing. Jisun Shin: Validation, Writing - Review & Editing. Jongbin Kim: Conceptualization, Methodology, Supervision, Project administration, Resources, Writing - Review & Editing

References

1. Walia T, Salami AA, Bashiri R, Hamoodi OM, Rashid F. A randomised controlled trial of three aesthetic full‑coronal restorations in primary maxillary teeth. Eur J Paediatr Dent 15:113–118. 2014;
2. Yin J, Li X, Zhang X, Yu S, Lai Y. Progress in sintering technology of transparent polycrystalline alumina ceramics. J Adv Dielectrics 14:2330002. 2024;
3. Ikesue A, Aung YL. Anisotropic alumina ceramics with isotropic optical properties. J Adv Ceram 12:72–81. 2023;
4. Zhao M, Sun Y, Zhang J, Zhang Y. Novel translucent and strong submicron alumina ceramics for dental restorations. J Dent Res 97:289–295. 2018;
5. Vijan K. Emerging trends and clinical recommendations for zirconia ceramic crowns: a concise review. Br Dent J 237:28–32. 2024;
6. Lundgren GP, Vestlund GI, Dahllöf G. Crown therapy in young individuals with amelogenesis imperfecta: long term follow‑up of a randomised controlled trial. J Dent 76:102–108. 2018;
7. Passos SP, Valandro LF, Bottino MA, Santos MJMC, Santos Jr GC. Shear bond strength of resin cement bonded to alumina ceramic after treatment by aluminum oxide sandblasting or silica coating. J Prosthodont 20:561–565. 2011;
8. Blatz MB, Sadan A, Kern M. Resin‑ceramic bonding: a review of the literature. J Prosthet Dent 89:268–274. 2003;
9. Friederich R, Kern M. Resin bond strength to densely sintered alumina ceramic. Int J Prosthodont 15:333–338. 2002;
10. Bindl A, Lüthy H, Mörmann WH. Thin‑wall ceramic CAD/CAM crown copings: strength and fracture pattern. J Oral Rehabil 33:520–528. 2006;
11. Lee JG, Park HW, Lee JH, Seo HW. Shear bonding strength of three cements luted on pediatric zirconia crowns and dentin of primary teeth. J Korean Acad Pediatr Dent 45:314–323. 2018;
12. Lüthy H, Loeffel O, Hämmerle CHF. Effect of thermocycling on bond strength of luting cements to zirconia ceramic. Dent Mater 22:195–200. 2006;
13. Piwowarczyk A, Lauer HC, Sorensen JA. In vitro shear bond strength of cementing agents to fixed‑prosthodontic restorative materials. J Prosthet Dent 92:265–273. 2004;
14. Ernst CP, Cohnen U, Stender E, Willershausen B. In vitro retentive strength of zirconium oxide ceramic crowns using different luting agents. J Prosthet Dent 93:551–558. 2005;
15. Palacios RP, Johnson GH, Phillips KM, Raigrodski AJ. Retention of zirconium oxide ceramic crowns with three types of cement. J Prosthet Dent 96:104–114. 2006;
16. Bhavana BL, Rupesh PL, Kataraki B. An in vitro comparison of the effect of various surface treatments on the tensile bond strength of three different luting cement to zirconia copings. J Indian Prosthodont Soc 19:26–32. 2019;
17. Park SJ, Lee JS. Effect of surface treatment on shear bond strength of relining material and 3D‑printed denture base. J Adv Prosthodont 14:262–272. 2022;
18. Solís Pinargote NW, Yanushevich O, Krikheli N, Smirnov A, Savilkin S, Grigoriev SN, Peretyagin P. Materials and methods for all‑ceramic dental restorations using computer‑aided design (CAD) and computer‑aided manufacturing (CAM) technologies - a brief review. Dent J (Basel) 12:47. 2024;
19. Ayman MT, Bae HM, Kwon H, Lee J, Yoon DH. Transparent polycrystalline γ‑AlON ceramics. Ceramist 23:244–260. 2020;
20. Awliya W, Odén A, Yaman P, Dennison JB, Razzoog ME. Shear bond strength of a resin cement to densely sintered high‑purity alumina with various surface conditions. Acta Odontol Scand 56:9–13. 1998;
21. Özcan M. Evaluation of alternative intra‑oral repair techniques for fractured ceramic‑fused‑to‑metal restorations. J Oral Rehabil 30:194–203. 2003;
22. Thompson JY, Stoner BR, Piascik JR, Smith R. Adhesion/cementation to zirconia and other non‑silicate ceramics: where are we now. Dent Mater 27:71–82. 2011;
23. Blatz MB, Sadan A, Martin J, Lang B. In vitro evaluation of shear bond strengths of resin to densely sintered high‑purity zirconium‑oxide ceramic after long‑term storage and thermal cycling. J Prosthet Dent 91:356–362. 2004;
24. Yun JY, Ha SR, Lee JB, Kim SH. Effect of sandblasting and various metal primers on the shear bond strength of resin cement to Y‑TZP ceramic. Dent Mater 26:650–658. 2010;
25. Phark JH, Duarte S Jr, Blatz M, Sadan A. An in vitro evaluation of the long‑term resin bond to a new densely sintered high‑purity zirconium‑oxide ceramic surface. J Prosthet Dent 101:29–38. 2009;
26. Valandro LF, Della Bona A, Bottino MA, Neisser MP. The effect of ceramic surface treatment on bonding to densely sintered alumina ceramic. J Prosthet Dent 93:253–259. 2005;
27. Lin J, Shinya A, Gomi H, Shinya A. Effect of self‑adhesive resin cement and tribochemical treatment on bond strength to zirconia. Int J Oral Sci 2:28–34. 2010;
28. Nagaoka N, Yoshihara K, Feitosa VP, Tamada Y, Irie M, Yoshida Y, Van Meerbeek B, Hayakawa S. Chemical interaction mechanism of 10‑MDP with zirconia. Sci Rep 7:45563. 2017;
29. Zhao R, Rupper P, Gaan S. Recent development in phosphonic acid‑based organic coatings on aluminum. Coatings 7:133. 2017;
30. Sciasci P, Abi‑Rached FO, Adabo GL, Baldissara P, Fonseca RG. Effect of surface treatments on the shear bond strength of luting cements to Y‑TZP ceramic. J Prosthet Dent 113:212–219. 2015;
31. Kim MJ, Kim YK, Kim KH, Kwon TY. Shear bond strengths of various luting cements to zirconia ceramic: surface chemical aspects. J Dent 39:795–803. 2011;
32. Marchan S, Coldero L, Whiting R, Barclay S. In vitro evaluation of the retention of zirconia‑based ceramic posts luted with glass ionomer and resin cements. Braz Dent J 16:213–217. 2005;
33. Aboushelib MN, Matinlinna JP, Salameh Z, Ounsi H. Innovations in bonding to zirconia‑based materials: Part I. Dent Mater 24:1268–1272. 2008;
34. Amaral R, Özcan M, Valandro LF, Balducci I, Bottino MA. Effect of conditioning methods on the microtensile bond strength of phosphate monomer‑based cement on zirconia ceramic in dry and aged conditions. J Biomed Mater Res B Appl Biomater 85:1–9. 2008;
35. Chang JC, Powers JM, Hart D. Bond strength of composite to alloy treated with bonding systems. J Prosthodont 2:110–114. 1993;
36. Kern M, Wegner SM. Bonding to zirconia ceramic: adhesion methods and their durability. Dent Mater 14:64–71. 1998;
37. International Organization for Standardization. ISO 10477 Dentistry‑Polymer‑based crown and bridge materials; 2004.

Article information Continued

Fig 1.

Disk-shaped submicron polycrystalline alumina ceramic specimen.

Fig 2.

Schematic diagram of the shear bond strength test.

UTM: universal testing machine.

Fig 3.

Effect of different surface treatments on the shear bond strength (MPa) of various luting cements. Groups sharing the same letter are not significantly different. Error bars represent standard deviation.

No: No treatment; Sb: Sandblasting; Ro: Rocatec treatment; GCF: GC Fuji I cement; RXL: RelyX Luting 2 cement; RXU: RelyX U200 cement.

Fig 4.

Effect of different luting cements on the shear bond strength (MPa) of surface-treated submicron polycrystalline alumina specimens. Groups sharing the same letter are not significantly different. Error bars represent standard deviation.

No: No treatment; Sb: Sandblasting; Ro: Rocatec treatment; GCF: GC Fuji I cement; RXL: RelyX Luting 2 cement; RXU: RelyX U200 cement.

Fig 5.

SEM images of surface-treated submicron polycrystalline alumina ceramic (magnification ×1,000). (A) No surface treatment, (B) Sandblasting, (C) Rocatec treatment.

Fig 6.

SEM images after the shear bond strength test showing failure mode on submicron polycrystalline alumina ceramic (magnification ×200). (A) Adhesive failure on surfaces with no treatment, (B) Mixed failure on surfaces treated by sandblasting, (C) Cohesive failure treated by Rocatec treatment.

Fig 7.

Comparison of the failure modes of polycrystalline alumina ceramics according to different surface treatments and luting cements.

No: No surface treatment; Sb: Sandblasting; Ro: Rocatec treatment; GCF: GC Fuji I cement; RXL: RelyX Luting 2 cement; RXU: RelyX U200 cement.

Table 1.

Compositions and manufacturers of cement used in this study

Material Material group Composition Manufacturer
GC Fuji I Glass ionomer cement Powder: aluminosilicate glass, polyacrylic acid GC Corporation, Tokyo, Japan
Liquid: polyacrylic acid, water
RelyX Luting 2 Resin-modified glass ionomer cement Paste A: fluoroaluminosilicate glass, proprietary reducing agent, 2-hydroxyethyl methacrylate, water, opacifying agent 3M ESPE, St. Paul, MN, USA
Paste B: methacrylated polycarboxylic acid, BisGMA, 2-hydroxyethyl methacrylate, water, potassium persulfate, zirconia silica filler
RelyX U200 Self-adhesive resin cement Base: methacrylate monomers containing phosphoric acid groups, methacrylate monomers, initiators, stabilizers, rheological additives 3M ESPE, St. Paul, MN, USA
Catalyst: methacrylate monomers, alkaline fillers, silanated fillers, initiator components, stabilizers, pigments, rheological additives, zirconia silica filler

Bis-GMA: bisphenol-A-glycidyl methacrylate.

Table 2.

Compositions and manufacturers of surface treatment materials in this study

Material Material group Composition Manufacturer
Rocatec Pre Sandblasting powder High-purity aluminum oxide (110 μm) 3M ESPE, St. Paul, MN, USA
Rocatec Plus Silica-coated powder Silica-modified aluminum oxide (110 μm) 3M ESPE, St. Paul, MN, USA
Monobond N Silane primer Ethanol, silane methacrylate, phosphoric acid methacrylate, sulfide methacrylate Ivoclar Vivadent, Schaan, Liechtenstein

Table 3.

Experimental group classification

Group Surface treatment Cement
No_GCF No treatment Gl cement (GC Fuji I)
No_RXL RMGI cement (RelyX Luting 2)
No_RXU Self-adhesive resin cement (RelyX U200)
Sb_GCF Sandblasting GI cement (GC Fuji I)
Sb_RXL RMGI cement (RelyX Luting 2)
Sb_RXU Self-adhesive resin cement (RelyX U200)
Ro_GCF Rocatec treatment GI cement (GC Fuji I)
Ro_RXL RMGI cement (RelyX Luting 2)
Ro_RXU Self-adhesive resin cement (RelyX U200)

GCF: GC Fuji I cement; RXL: RelyX Luting 2 cement; RXU: RelyX U200 cement; GI: glass ionomer; RMGI: resin-modified glass ionomer.

Table 4.

Shear bond strength (MPa) of various cements according to surface treatment

Surface treatment GCF RXL RXU
No treatment 0.07 ± 0.06A,a 0.34 ± 0.13B,a 1.47 ± 0.24C,a
Sandblasting 0.14 ± 0.07A,a 0.76 ± 0.15B,b 6.30 ± 1.45C,b
Rocatec treatment 0.15 ± 0.08A,a 1.59 ± 0.42B,c 10.24 ± 0.93C,c

Kruskal-Wallis test and Bonferroni test.

Different upper letters represent statistical significance (p < 0.017) in the same row and different lower letters represent statistical significance in the same column (p < 0.017).

GCF: GC Fuji I cement; RXL: RelyX Luting 2 cement; RXU: RelyX U200 cement.